CC;
What do you recommend be placed under the bamboo and on top of the concrete floor assuming we get good results from tests.. (Bamboo is a floating floor ..no sub wood floor in place) Currently Aquabar"B". SHould the RH test be done in addition to CACL?

11-14-2010, 10:18 AM #12
CC Solutions Concrete Moisture Evangelist *******
Status: Offline Posts:1,067 Threads:69 Joined:Dec 2009
If the results are within the parameters of the manufacturer, just follow the manufacturer's advice for an underlayment. The foam should be just fine.

JD Grafton
Concrete Answers for Flooring Problems
JGrafton@ccsolves.com

11-18-2010, 05:01 PM #13
Justin Newbie *
Status: Offline Posts:1 Threads:0 Joined:Nov 2010
I just finished watching Howard Kanare's videos on YouTube and I wouldn't trust either the CaCl or moisture meters. You want to measure the RH inside the slab, not the surface like the first two tests.

11-19-2010, 05:31 PM #14
CC Solutions Concrete Moisture Evangelist *******
Status: Offline Posts:1,067 Threads:69 Joined:Dec 2009
(11-18-2010, 05:01 PM)Justin Wrote:  I just finished watching Howard Kanare's videos on YouTube and I wouldn't trust either the CaCl or moisture meters. You want to measure the RH inside the slab, not the surface like the first two tests.

Justin, you have good cause to fear MVER testing and the EI testers! But keep in mind RH tests are not valid if a mitigation system is in place. A quality mitigation system will reduce MVER to acceptable levels while the internal RH remains high for many many years.

One must look at the entire picture to make rational decisions on how to proceed with any slab. Wink

JD Grafton
Concrete Answers for Flooring Problems
JGrafton@ccsolves.com

11-20-2010, 01:08 PM #15
Ernesto Concrete Moisture Expert *****
Status: Offline Posts:606 Threads:33 Joined:Sep 2009
Lots of those 2 in 1 cushion/vapor retarders can only handle up to 5lbs of vapor emissions measure with a cacl test.

Also...not to rain on anyones parade...just because the rh may be a tad high does not mean thats what is going to come out of the surface. Lots of variables like mix ratios, additives, steel trowel finishes all add up.

If your already having issues I'd go the extra six cents with a layer of 6 mil plastic under the 2 an 1. Hope I ain't to late.......Tongue

Stephen Perrera dba
Top Floor Installation Co.
http://www.tucsonazflooring.com
http://www.floorsavior.com

11-20-2010, 02:28 PM #16
sbhtennis Newbie *
Status: Offline Posts:11 Threads:1 Joined:Oct 2010
Thanks everyone for your ideas. We are going to do CACL in two or three other places on the floor + a RH tests. This way if they are truly high the installer will be on board with doing the right solution... whether it be a sealer or the 6 mil plastic or both. The unfortunate thing is me having to spend $ on these tests, but I suppose in the end it will then be worth it so that we have actual facts. I'll keep you all posted.

12-04-2010, 11:02 AM #17
eaadams Concrete Moisture Expert *****
Status: Offline Posts:600 Threads:88 Joined:Jul 2010
6 mil plastic ....

We use the equivalent of stego & use an asphaltic tape on the seams. 6mil can still have a very high perm rating.

12-04-2010, 04:03 PM #18
sbhtennis Newbie *
Status: Offline Posts:11 Threads:1 Joined:Oct 2010
would you use this in addition to the Aquabar "B" over the concrete floor. We got Cacl test of 4.04% . Does that sound OK?

12-05-2010, 07:15 AM #19
CC Solutions Concrete Moisture Evangelist *******
Status: Offline Posts:1,067 Threads:69 Joined:Dec 2009
4% MVER is very low, and again, I always suspect inaccurate results using CaCl tests.

If you can eliminate the possibility of moisture introduced from above (washing, mopping etc) and extreme ambient RH swings from heating and cooling (the bamboo is a sponge! ) I would then suspect the substrate even though the Aquabar is in place.

JD Grafton
Concrete Answers for Flooring Problems
JGrafton@ccsolves.com

12-05-2010, 12:41 PM #20
eaadams Concrete Moisture Expert *****
Status: Offline Posts:600 Threads:88 Joined:Jul 2010
FYI http://www.fortifiber.com/pdf/data_sheets/DS_aquabar_b.pdf

<1 perm. (not too specific)








Possibly Related Threads...
Thread / Author Replies / Views Last Post
3 Replies 8,588 Views
Last Post by Rubensgt40
07-05-2014, 03:18 AM
13 Replies 28,197 Views
Last Post by eaadams
05-19-2014, 10:55 AM
2 Replies 7,336 Views
Last Post by Rubensgt40
05-10-2014, 08:07 PM
2 Replies 10,074 Views
Last Post by eaadams
09-27-2013, 10:26 AM
4 Replies 15,143 Views
Last Post by CC Solutions
09-18-2012, 06:11 PM
23 Replies 73,810 Views
Last Post by foxgeorge
12-15-2011, 01:20 AM
5 Replies 17,117 Views
Last Post by Ernesto
08-14-2011, 08:43 PM
8 Replies 25,487 Views
Last Post by CC Solutions
06-09-2011, 06:09 AM
17 Replies 49,811 Views
Last Post by CC Solutions
04-01-2011, 09:02 PM

Users browsing this thread:
1 Guest(s)