Status: Offline Posts:600 Threads:88 Joined:Jul 2010
All tests done with Wagner 4.0.

Date / test site / RH / Temp

7-11 / #1 / 94 / 73
7-17 / #1 / 94 / not recorded
[heat turned on, air moved, floor received a light shotblast to a CSP of no more than 2]
7-30 / #1 / 94 / 79
8-07 - no test

7-11 / #2 / 96 / 73
7-17 / #2 / 91 / not recorded
[heat turned on, air moved, floor received a light shotblast to a CSP of no more than 2]
7-30 / #2 / [no reading / debris]
[hole vacuumed out of debris @ time of test]
8-07 - no test

7-11 / #3 / 91 / 74
7-17 / #3 / 99 / not recorded
[heat turned on, air moved, floor received a light shotblast to a CSP of no more than 2]
7-30 / #3 / 99 / 79
8-07 / #3 / 94 / 76

7-11 / #4 / 92 / 72
7-17 / #4 / 92 / not recorded
[heat turned on, air moved, floor received a light shotblast to a CSP of no more than 2]
7-30 / #4 / 91 / 79
8-07 / #4 / 91 / 75

7-11 / #5 / 99 / 72
7-17 / #5 / 99 / not recorded
[heat turned on, air moved, floor received a light shotblast to a CSP of no more than 2]
7-30 / #5 / 94 / 79
8-07 - no test


Obviously the slab temp went up when we cranked the HVAC. I think removing the old adhesive with the light shotblast helped a lot to let moisture out just over one month.








Messages In This Thread
Heat, move air, shotblast = lower results - eaadams - 08-07-2013, 12:35 PM
RE: Heat, move air, shotblast = lower results - CC Solutions - 09-01-2013, 07:56 AM

Possibly Related Threads...
Thread / Author Replies / Views Last Post
7 Replies 24,334 Views
Last Post by Rubensgt40
05-09-2012, 04:35 PM
11 Replies 36,450 Views
Last Post by CC Solutions
10-28-2011, 02:12 PM

Users browsing this thread:
1 Guest(s)