05-01-2013, 07:20 AM #36
jim decker Concrete Moisture Enthusiast *
Status: Offline Posts:42 Threads:4 Joined:Nov 2011
REGARDING THE MAPLE INCREASE IN RH SEE BELOW:
The MFMA has revised the acceptable level of relative humidity in a concrete slab for non-glue down floor systems from <=80% to <=85%. This revision was made in response to feedback received from our contractor members during the past several years. The MFMA Technical Committee reviewed this information and felt confident raising the level to 85% based on contractor experience with successful installation of maple systems over concrete slabs with relative humidity level in excess of 80%.
MFMA continues to only recognize the testing of a concrete slab’s relative humidity levels using the most recent version of ASTM F2170. Please refer to the instructions of the manufacturer’s relative humidity test kit for details on how to administer the test correctly. MFMA now recommends that the relative humidity level for a concrete slag for a non-glue-down maples floor system is 85% or lower and for glue down systems the relative humidity remains at 75% or lower before installation. For concrete relative humidity conditions above MFMA”s recommendation consult your MFMA Sport Floor Contractor or your MFMA Manufacturer.
So this means a sports floor over screeds not glued to the floor 85% is allowable BUT for glue down floors 80% is the requirement. Remember this is for sports floors. Manufacturers of Maple floors for other than sports floors the requirement by all mfg’s of residential is 75% relative humidity.
One must be careful about what exactly is the situation!








Messages In This Thread
RH in Concrete for Wood Floor with Vapor Membrane - eaadams - 06-14-2012, 10:31 AM
RE: RH in Concrete for Wood Floor with Vapor Membrane - CC Solutions - 06-14-2012, 10:51 AM
RE: RH in Concrete for Wood Floor with Vapor Membrane - eaadams - 06-14-2012, 10:56 AM
RE: RH in Concrete for Wood Floor with Vapor Membrane - CC Solutions - 06-14-2012, 10:59 AM
RE: RH in Concrete for Wood Floor with Vapor Membrane - eaadams - 06-14-2012, 12:20 PM
RE: RH in Concrete for Wood Floor with Vapor Membrane - CCR - 06-14-2012, 05:56 PM
RE: RH in Concrete for Wood Floor with Vapor Membrane - CC Solutions - 06-15-2012, 07:01 AM
RE: RH in Concrete for Wood Floor with Vapor Membrane - Rubensgt40 - 06-18-2012, 04:55 PM
RE: RH in Concrete for Wood Floor with Vapor Membrane - CC Solutions - 06-18-2012, 05:55 PM
RE: RH in Concrete for Wood Floor with Vapor Membrane - eaadams - 06-19-2012, 11:49 AM
RE: RH in Concrete for Wood Floor with Vapor Membrane - CC Solutions - 06-19-2012, 01:38 PM
RE: RH in Concrete for Wood Floor with Vapor Membrane - Ernesto - 06-20-2012, 08:00 PM
RE: RH in Concrete for Wood Floor with Vapor Membrane - eaadams - 06-25-2012, 02:02 PM
RE: RH in Concrete for Wood Floor with Vapor Membrane - simmonsviolet - 08-22-2012, 04:44 AM
RE: RH in Concrete for Wood Floor with Vapor Membrane - CC Solutions - 08-22-2012, 06:37 AM
RE: RH in Concrete for Wood Floor with Vapor Membrane - Ernesto - 08-22-2012, 10:50 AM
RE: RH in Concrete for Wood Floor with Vapor Membrane - Rubensgt40 - 08-23-2012, 04:17 PM
RE: RH in Concrete for Wood Floor with Vapor Membrane - Ernesto - 08-23-2012, 07:25 PM
RE: RH in Concrete for Wood Floor with Vapor Membrane - CC Solutions - 08-24-2012, 05:58 AM
RE: RH in Concrete for Wood Floor with Vapor Membrane - Ernesto - 08-24-2012, 12:21 PM
RE: RH in Concrete for Wood Floor with Vapor Membrane - jim decker - 03-17-2013, 07:40 PM
RE: RH in Concrete for Wood Floor with Vapor Membrane - Rubensgt40 - 03-17-2013, 08:25 PM
RE: RH in Concrete for Wood Floor with Vapor Membrane - jim decker - 03-18-2013, 08:44 PM
RE: RH in Concrete for Wood Floor with Vapor Membrane - CC Solutions - 03-19-2013, 06:34 AM
RE: RH in Concrete for Wood Floor with Vapor Membrane - jim decker - 03-22-2013, 07:20 AM
RE: RH in Concrete for Wood Floor with Vapor Membrane - jim decker - 03-22-2013, 01:36 PM
RE: RH in Concrete for Wood Floor with Vapor Membrane - CC Solutions - 03-22-2013, 02:19 PM
RE: RH in Concrete for Wood Floor with Vapor Membrane - Rubensgt40 - 03-25-2013, 05:20 PM
RE: RH in Concrete for Wood Floor with Vapor Membrane - CC Solutions - 03-25-2013, 05:44 PM
RE: RH in Concrete for Wood Floor with Vapor Membrane - Rubensgt40 - 03-25-2013, 08:47 PM
RE: RH in Concrete for Wood Floor with Vapor Membrane - jim decker - 03-26-2013, 06:13 AM
RE: RH in Concrete for Wood Floor with Vapor Membrane - CC Solutions - 03-26-2013, 06:27 AM
RE: RH in Concrete for Wood Floor with Vapor Membrane - Ernesto - 03-30-2013, 11:33 AM
RE: RH in Concrete for Wood Floor with Vapor Membrane - eaadams - 04-29-2013, 03:58 PM
RE: RH in Concrete for Wood Floor with Vapor Membrane - jim decker - 04-30-2013, 08:02 AM
RE: RH in Concrete for Wood Floor with Vapor Membrane - jim decker - 05-01-2013, 07:20 AM

Possibly Related Threads...
Thread / Author Replies / Views Last Post
4 Replies 13,993 Views
Last Post by Ashok Kakade
05-20-2014, 12:00 PM
13 Replies 36,067 Views
Last Post by eaadams
05-19-2014, 10:55 AM
9 Replies 44,276 Views
Last Post by eaadams
11-08-2013, 01:41 PM
21 Replies 82,288 Views
Last Post by CCR
07-19-2013, 05:14 PM
4 Replies 16,920 Views
Last Post by eaadams
01-30-2013, 04:43 PM
5 Replies 21,145 Views
Last Post by CC Solutions
12-15-2012, 06:46 AM
32 Replies 103,810 Views
Last Post by CC Solutions
05-08-2012, 07:04 AM
2 Replies 12,062 Views
Last Post by Ernesto
04-01-2012, 09:08 AM
0 Replies 6,648 Views
Last Post by eaadams
03-23-2012, 09:40 AM
2 Replies 14,320 Views
Last Post by eaadams
12-23-2011, 12:06 PM

Users browsing this thread:
1 Guest(s)