Hi, I'm new to using rapid RH and concrete moisture testing and would appreciate any feedback on the following:
Conditions:
-New 2500sq.ft. slab 6" thick installed over vapor barrier over 12" gravel foundation.
-trowel finished with no other products added (no sealer or other)
-installed 3 RH probes at 40% depth after 1 month of pour. Sensors read 97% after 1 hour and 99% ever since.
-Its now been almost 3 months since the end of the water cure and still 99%RH from all 3 probes
-The RH in the gym was about 50% and is now 30% for about a month already. Temp. of gym has been around 70 F
Questions:
-Is it normal to still have 99% while other test types have shown a drop?
-Are the probes malfunctioning and should I have waited longer prior to installing them?
-Should I go ahead and install another probe to be sure of the readings?

Thanks.








Messages In This Thread
High Rapid RH readings?? - ddemento - 11-03-2011, 12:13 PM
RE: High Rapid RH readings?? - eaadams - 11-03-2011, 12:33 PM
RE: High Rapid RH readings?? - CC Solutions - 11-03-2011, 04:20 PM
RE: High Rapid RH readings?? - ddemento - 11-07-2011, 12:58 PM
RE: High Rapid RH readings?? - CC Solutions - 11-07-2011, 01:05 PM
RE: High Rapid RH readings?? - eaadams - 11-07-2011, 01:20 PM
RE: High Rapid RH readings?? - CC Solutions - 11-07-2011, 01:36 PM
RE: High Rapid RH readings?? - eaadams - 11-07-2011, 01:52 PM
RE: High Rapid RH readings?? - CC Solutions - 11-07-2011, 02:01 PM
RE: High Rapid RH readings?? - Ernesto - 11-07-2011, 07:27 PM
RE: High Rapid RH readings?? - eaadams - 11-07-2011, 08:33 PM
RE: High Rapid RH readings?? - CC Solutions - 11-08-2011, 07:31 AM
RE: High Rapid RH readings?? - eaadams - 11-08-2011, 09:38 AM
RE: High Rapid RH readings?? - CC Solutions - 11-08-2011, 09:58 AM
RE: High Rapid RH readings?? - eaadams - 11-08-2011, 10:11 AM
RE: High Rapid RH readings?? - CC Solutions - 11-08-2011, 10:28 AM
RE: High Rapid RH readings?? - ddemento - 11-09-2011, 05:00 AM
RE: High Rapid RH readings?? - CC Solutions - 11-09-2011, 07:38 AM
RE: High Rapid RH readings?? - eaadams - 11-09-2011, 08:20 PM
RE: High Rapid RH readings?? - ddemento - 11-11-2011, 11:07 AM
RE: High Rapid RH readings?? - CC Solutions - 11-11-2011, 11:18 AM
RE: High Rapid RH readings?? - eaadams - 11-11-2011, 11:23 AM
RE: High Rapid RH readings?? - Ernesto - 11-11-2011, 04:36 PM
RE: High Rapid RH readings?? - eaadams - 11-11-2011, 08:49 PM
RE: High Rapid RH readings?? - CC Solutions - 11-12-2011, 03:44 PM
RE: High Rapid RH readings?? - Ernesto - 11-12-2011, 05:07 PM
RE: High Rapid RH readings?? - CC Solutions - 11-12-2011, 05:13 PM
RE: High Rapid RH readings?? - Ernesto - 11-12-2011, 05:45 PM
RE: High Rapid RH readings?? - ddemento - 11-16-2011, 10:05 AM
RE: High Rapid RH readings?? - eaadams - 11-16-2011, 10:50 AM
RE: High Rapid RH readings?? - CC Solutions - 11-16-2011, 11:04 AM
RE: High Rapid RH readings?? - eaadams - 11-16-2011, 11:32 AM
RE: High Rapid RH readings?? - CC Solutions - 11-16-2011, 11:53 AM
RE: High Rapid RH readings?? - ddemento - 11-16-2011, 01:25 PM
RE: High Rapid RH readings?? - CC Solutions - 11-16-2011, 02:18 PM
RE: High Rapid RH readings?? - Rubensgt40 - 11-16-2011, 03:34 PM
RE: High Rapid RH readings?? - eaadams - 11-16-2011, 04:28 PM
RE: High Rapid RH readings?? - Ernesto - 11-16-2011, 05:03 PM
RE: High Rapid RH readings?? - CC Solutions - 11-16-2011, 05:23 PM
RE: High Rapid RH readings?? - eaadams - 11-16-2011, 06:21 PM
RE: High Rapid RH readings?? - Ernesto - 11-16-2011, 06:43 PM
RE: High Rapid RH readings?? - ddemento - 11-17-2011, 06:16 AM
RE: High Rapid RH readings?? - CC Solutions - 11-17-2011, 08:12 AM
RE: High Rapid RH readings?? - eaadams - 11-17-2011, 10:13 AM
RE: High Rapid RH readings?? - Ernesto - 11-17-2011, 04:58 PM
RE: High Rapid RH readings?? - ddemento - 12-08-2011, 12:03 PM
RE: High Rapid RH readings?? - Ernesto - 12-08-2011, 12:48 PM
RE: High Rapid RH readings?? - CC Solutions - 12-08-2011, 12:58 PM
RE: High Rapid RH readings?? - eaadams - 12-08-2011, 05:55 PM
RE: High Rapid RH readings?? - Ernesto - 12-08-2011, 06:03 PM

Possibly Related Threads...
Thread / Author Replies / Views Last Post
4 Replies 5,472 Views
Last Post by eaadams
05-04-2016, 08:39 PM
3 Replies 16,423 Views
Last Post by CC Solutions
08-20-2012, 07:07 PM
15 Replies 57,791 Views
Last Post by CC Solutions
01-15-2012, 06:33 PM
64 Replies 186,961 Views
Last Post by CC Solutions
11-17-2011, 07:56 AM
4 Replies 16,368 Views
Last Post by CC Solutions
08-19-2011, 07:13 AM
6 Replies 21,755 Views
Last Post by CC Solutions
11-19-2010, 05:26 PM
 high rh in concrete
chas04344
2 Replies 14,699 Views
Last Post by chas04344
09-11-2009, 07:33 PM
1 Replies 12,024 Views
Last Post by rthompson
10-15-2008, 11:00 AM

Users browsing this thread:
1 Guest(s)