This is leveling 101.. You don't use warm water to mix self-leveling underlayments. Well I set up the job for a second floor pour at a local hospital. The closest water was an outside water bib on first floor. I had my guys run the hose up the wall, across the roof and through an access door to a hallway that led to our area.

The work began and I noticed right away that the material didn't self heal like normal. I had a shortened flow time between pours to blend the joints. The material set up really fast in the sunlit areas. Not until the entire 100 bags were down did it dawn on me that the hose running across the roof was warming the water. Luckily the roof was white rubber, but the green hose still absorbed radiant heat.

The job turned out not as good as we normally do, and I felt terrible. I talked with the flooring sub and asked him to evaluate the underlayment and let me know what his guys have to do to make it right. This bonehead move will cost me some money, but worse than that is it hurts my reputation. Sad

JD Grafton
Concrete Answers for Flooring Problems
JGrafton@ccsolves.com








Messages In This Thread
Self-leveling concrete - My bonehead mistake - CC Solutions - 08-21-2011, 08:20 AM
RE: Self-leveling concrete - My bonehead mistake - Ernesto - 08-21-2011, 04:36 PM
RE: Self-leveling concrete - My bonehead mistake - CC Solutions - 08-21-2011, 05:38 PM
RE: Self-leveling concrete - My bonehead mistake - Ernesto - 08-21-2011, 05:49 PM
RE: Self-leveling concrete - My bonehead mistake - CC Solutions - 08-21-2011, 06:09 PM
RE: Self-leveling concrete - My bonehead mistake - Ernesto - 08-22-2011, 04:46 PM
RE: Self-leveling concrete - My bonehead mistake - CC Solutions - 08-22-2011, 09:22 PM
RE: Self-leveling concrete - My bonehead mistake - eaadams - 08-25-2011, 11:28 AM
RE: Self-leveling concrete - My bonehead mistake - CC Solutions - 08-25-2011, 04:37 PM
RE: Self-leveling concrete - My bonehead mistake - eaadams - 08-25-2011, 05:42 PM
RE: Self-leveling concrete - My bonehead mistake - rthompson - 08-26-2011, 01:59 PM
RE: Self-leveling concrete - My bonehead mistake - CC Solutions - 08-26-2011, 02:36 PM
RE: Self-leveling concrete - My bonehead mistake - rthompson - 08-26-2011, 03:24 PM
RE: Self-leveling concrete - My bonehead mistake - amele001 - 08-27-2011, 02:28 PM
RE: Self-leveling concrete - My bonehead mistake - CC Solutions - 08-28-2011, 01:54 PM
RE: Self-leveling concrete - My bonehead mistake - rthompson - 08-28-2011, 02:34 PM
RE: Self-leveling concrete - My bonehead mistake - CC Solutions - 08-28-2011, 04:18 PM
RE: Self-leveling concrete - My bonehead mistake - EWagner - 08-28-2011, 05:22 PM
RE: Self-leveling concrete - My bonehead mistake - CC Solutions - 08-28-2011, 06:46 PM
RE: Self-leveling concrete - My bonehead mistake - Ernesto - 08-28-2011, 07:13 PM
RE: Self-leveling concrete - My bonehead mistake - CC Solutions - 08-29-2011, 05:47 AM
RE: Self-leveling concrete - My bonehead mistake - eaadams - 08-31-2011, 11:44 AM
RE: Self-leveling concrete - My bonehead mistake - CC Solutions - 08-31-2011, 03:22 PM
RE: Self-leveling concrete - My bonehead mistake - rthompson - 08-31-2011, 11:40 PM
RE: Self-leveling concrete - My bonehead mistake - eaadams - 09-07-2011, 09:09 AM
RE: Self-leveling concrete - My bonehead mistake - CC Solutions - 09-07-2011, 09:53 AM
RE: Self-leveling concrete - My bonehead mistake - eaadams - 09-15-2011, 10:22 AM
RE: Self-leveling concrete - My bonehead mistake - Ernesto - 09-15-2011, 12:27 PM
RE: Self-leveling concrete - My bonehead mistake - eaadams - 09-15-2011, 12:56 PM
RE: Self-leveling concrete - My bonehead mistake - CC Solutions - 09-15-2011, 01:06 PM
RE: Self-leveling concrete - My bonehead mistake - rthompson - 09-19-2011, 12:30 PM
RE: Self-leveling concrete - My bonehead mistake - CC Solutions - 09-19-2011, 02:06 PM
RE: Self-leveling concrete - My bonehead mistake - eaadams - 09-19-2011, 02:08 PM
RE: Self-leveling concrete - My bonehead mistake - CC Solutions - 09-19-2011, 02:14 PM
RE: Self-leveling concrete - My bonehead mistake - eaadams - 09-20-2011, 09:38 AM
RE: Self-leveling concrete - My bonehead mistake - CC Solutions - 09-20-2011, 09:57 AM
RE: Self-leveling concrete - My bonehead mistake - eaadams - 09-20-2011, 10:01 AM
RE: Self-leveling concrete - My bonehead mistake - CC Solutions - 09-20-2011, 10:07 AM

Possibly Related Threads...
Thread / Author Replies / Views Last Post
4 Replies 11,157 Views
Last Post by Ashok Kakade
05-20-2014, 12:00 PM
13 Replies 28,034 Views
Last Post by eaadams
05-19-2014, 10:55 AM
9 Replies 39,766 Views
Last Post by eaadams
11-08-2013, 01:41 PM
6 Replies 14,908 Views
Last Post by CC Solutions
05-27-2013, 10:05 AM
35 Replies 100,527 Views
Last Post by jim decker
05-01-2013, 07:20 AM
4 Replies 14,397 Views
Last Post by eaadams
01-30-2013, 04:43 PM
32 Replies 91,813 Views
Last Post by CC Solutions
05-08-2012, 07:04 AM
0 Replies 5,795 Views
Last Post by eaadams
03-23-2012, 09:40 AM
23 Replies 73,586 Views
Last Post by foxgeorge
12-15-2011, 01:20 AM
12 Replies 41,391 Views
Last Post by CC Solutions
06-21-2011, 11:47 AM

Users browsing this thread:
2 Guest(s)