This is leveling 101.. You don't use warm water to mix self-leveling underlayments. Well I set up the job for a second floor pour at a local hospital. The closest water was an outside water bib on first floor. I had my guys run the hose up the wall, across the roof and through an access door to a hallway that led to our area.

The work began and I noticed right away that the material didn't self heal like normal. I had a shortened flow time between pours to blend the joints. The material set up really fast in the sunlit areas. Not until the entire 100 bags were down did it dawn on me that the hose running across the roof was warming the water. Luckily the roof was white rubber, but the green hose still absorbed radiant heat.

The job turned out not as good as we normally do, and I felt terrible. I talked with the flooring sub and asked him to evaluate the underlayment and let me know what his guys have to do to make it right. This bonehead move will cost me some money, but worse than that is it hurts my reputation. Sad

JD Grafton
Concrete Answers for Flooring Problems
JGrafton@ccsolves.com

08-21-2011, 04:36 PM #2
Ernesto Concrete Moisture Expert *****
Status: Offline Posts:606 Threads:33 Joined:Sep 2009
If it were me I'd tell you to take it all out and do it over. Tongue What do you mean having him tell you what to have his guys do? Can you say DEMO TIME!

Any installer would know warm water makes any patch or SLC set up super fast. You of course realize what happens to that stuff when it sets to quick, doncha? ...making scary face.

Me, I carry bags of ice and make ice water. Course I do not do commercial so in that case you woulda needed a truck full of ice.

Stephen Perrera dba
Top Floor Installation Co.
http://www.tucsonazflooring.com
http://www.floorsavior.com

08-21-2011, 05:38 PM #3
CC Solutions Concrete Moisture Evangelist *******
Status: Offline Posts:1,067 Threads:69 Joined:Dec 2009
I know... what was I thinking???
The job isn't bad, but it's not perfect. It is 3500sf and there are two cold joints between two big areas, and I wish I could have blended them better.

The installer thinks it will be just a little touch up, but I want to cover his costs on anything unusual.

JD Grafton
Concrete Answers for Flooring Problems
JGrafton@ccsolves.com

08-21-2011, 05:49 PM #4
Ernesto Concrete Moisture Expert *****
Status: Offline Posts:606 Threads:33 Joined:Sep 2009
Are you going to do a psi test on it?

Stephen Perrera dba
Top Floor Installation Co.
http://www.tucsonazflooring.com
http://www.floorsavior.com

08-21-2011, 06:09 PM #5
CC Solutions Concrete Moisture Evangelist *******
Status: Offline Posts:1,067 Threads:69 Joined:Dec 2009
A tensile test? No, I was gone already. I asked if the flooring company wanted me to come back immediately to start testing, but they are familiar with underlayments and were not concerned.
We have a trusting relationship. Wink

JD Grafton
Concrete Answers for Flooring Problems
JGrafton@ccsolves.com

08-22-2011, 04:46 PM #6
Ernesto Concrete Moisture Expert *****
Status: Offline Posts:606 Threads:33 Joined:Sep 2009
Course they are not concerned. They want to go in and get the floor down and make some cash. If anything happens you know who they will blame.

Stephen Perrera dba
Top Floor Installation Co.
http://www.tucsonazflooring.com
http://www.floorsavior.com

08-22-2011, 09:22 PM #7
CC Solutions Concrete Moisture Evangelist *******
Status: Offline Posts:1,067 Threads:69 Joined:Dec 2009
Well anyone I work with is a team member, and they want no problems any more than I do. I trust they will evaluate the underlayment and act accordingly. I have repairs many substandard floors for them before....

Even though mine was not as good as I wanted it, it was still probably better than 95% of them out there.... Tongue

JD Grafton
Concrete Answers for Flooring Problems
JGrafton@ccsolves.com

08-25-2011, 11:28 AM #8
eaadams Concrete Moisture Expert *****
Status: Offline Posts:600 Threads:88 Joined:Jul 2010
(08-21-2011, 06:09 PM)CC Solutions Wrote:  A tensile test?

For those interested in doing their own tensile tests, I learned to use this on underlayment from the CTS Cement people, also have seen CTL use it on Koster jobs to test adhesion of the Koster: http://www.elcometer.com/en/elcometer-106/6-coating-on-concrete-adhesion-tester.html

I do not know how to do a 'psi' test on an installed underlayment.

08-25-2011, 04:37 PM #9
CC Solutions Concrete Moisture Evangelist *******
Status: Offline Posts:1,067 Threads:69 Joined:Dec 2009
That's the one I use.... They don't cost too much and they work well.

JD Grafton
Concrete Answers for Flooring Problems
JGrafton@ccsolves.com

08-25-2011, 05:42 PM #10
eaadams Concrete Moisture Expert *****
Status: Offline Posts:600 Threads:88 Joined:Jul 2010
It is what UCLA trains the PE's to use.

But it is UCLA.... almost as bad as USC or ASU.

Go Davis Aggies Smile or CAL :|








Possibly Related Threads...
Thread / Author Replies / Views Last Post
4 Replies 11,225 Views
Last Post by Ashok Kakade
05-20-2014, 12:00 PM
13 Replies 28,201 Views
Last Post by eaadams
05-19-2014, 10:55 AM
9 Replies 39,873 Views
Last Post by eaadams
11-08-2013, 01:41 PM
6 Replies 14,984 Views
Last Post by CC Solutions
05-27-2013, 10:05 AM
35 Replies 100,852 Views
Last Post by jim decker
05-01-2013, 07:20 AM
4 Replies 14,455 Views
Last Post by eaadams
01-30-2013, 04:43 PM
32 Replies 92,100 Views
Last Post by CC Solutions
05-08-2012, 07:04 AM
0 Replies 5,820 Views
Last Post by eaadams
03-23-2012, 09:40 AM
23 Replies 73,813 Views
Last Post by foxgeorge
12-15-2011, 01:20 AM
12 Replies 41,522 Views
Last Post by CC Solutions
06-21-2011, 11:47 AM

Users browsing this thread:
1 Guest(s)