I visited a job where the slab is wet under the vinyl. The hospital has tried every repair the installer has recommended. They have changed glues, installed new patches, changed some areas to rubber... nothing works.

I looked at the job and told them it sure looks like a moisture issue. I was shown test results from a local engineering firm claiming the slab RH is in the 50's percent range. The report was done with fancy letterhead on fancy paper, but many important details were missing, the ASTM was not followed, and the equipment used I absolutely despise Tongue. The hospital paid a lot of money for the testing.

Because of all the repairs and existing floor bubbles the hospital facilities guy was under a lot of pressure to figure this out! He was being given so many conflicting reports, he was truly beside himself. I told the facilities engineer I would conduct RH testing for free, no strings attached, just so we could have solid results to look at. The job is several hours away from my office and he'd like me to do my testing at 6am. Big Grin

But you know what? No matter what happens we'll all learn something, and if things go the way I think they will, I'll prove my value to the facility and make some new friends in the industry. That is priceless!!

JD Grafton
Concrete Answers for Flooring Problems
JGrafton@ccsolves.com

04-01-2011, 09:26 AM #2
eaadams Concrete Moisture Expert *****
Status: Offline Posts:600 Threads:88 Joined:Jul 2010
As long as they don't put the work out to bid that sounds good. I have had school officials do the same thing and show zero loyalty afterward

04-01-2011, 09:35 AM #3
CC Solutions Concrete Moisture Evangelist *******
Status: Offline Posts:1,067 Threads:69 Joined:Dec 2009
Well, even if they have someone else do the work, at least if my predictions are correct and I can show how the trusted 'expert' has done them a disservice, I think I will be happy.

I was recommended by an engineer at the state, so as long as I perform admirably I will improve my reputation. And sometimes that's all I can ask for.

JD Grafton
Concrete Answers for Flooring Problems
JGrafton@ccsolves.com

04-01-2011, 03:38 PM #4
Ernesto Concrete Moisture Expert *****
Status: Offline Posts:606 Threads:33 Joined:Sep 2009
Arn't schools required to have bids?

Stephen Perrera dba
Top Floor Installation Co.
http://www.tucsonazflooring.com
http://www.floorsavior.com

04-01-2011, 09:04 PM #5
CC Solutions Concrete Moisture Evangelist *******
Status: Offline Posts:1,067 Threads:69 Joined:Dec 2009
I suppose they are. I was a consultant though. When nobody can figure out the problem, I guess they just keep asking people for an answer.

JD Grafton
Concrete Answers for Flooring Problems
JGrafton@ccsolves.com

04-02-2011, 07:44 AM #6
Ernesto Concrete Moisture Expert *****
Status: Offline Posts:606 Threads:33 Joined:Sep 2009
Problem is with some people is that they want you to come over and look at it for them for free. Free don't pay the bills. And you can't tell them exactly what the problem is by looking at it.....let me rephrase that.....a concrete guru can Smile but why would you since they have the answer they wanted and now will try another avenue to fitz it.

Stephen Perrera dba
Top Floor Installation Co.
http://www.tucsonazflooring.com
http://www.floorsavior.com

susiehaynes Show this Post
04-02-2011, 09:49 PM #7
susiehaynes Unregistered
 
(04-02-2011, 07:44 AM)Ernesto Wrote:  Problem is with some people is that they want you to come over and look at it for them for free. Free don't pay the bills. And you can't tell them exactly what the problem is by looking at it.....let me rephrase that.....a concrete guru can Smile but why would you since they have the answer they wanted and now will try another avenue to fitz it.

can't tell much but to agree with you..

04-03-2011, 05:39 PM #8
CC Solutions Concrete Moisture Evangelist *******
Status: Offline Posts:1,067 Threads:69 Joined:Dec 2009
(04-02-2011, 07:44 AM)Ernesto Wrote:  Problem is with some people is that they want you to come over and look at it for them for free. Free don't pay the bills. And you can't tell them exactly what the problem is by looking at it.....let me rephrase that.....a concrete guru can Smile but why would you since they have the answer they wanted and now will try another avenue to fitz it.

I always go for free.... And sometimes I will do RH and CaCl testing for free. I usually start balking on the third or fourth visit if I don't feel like I'm going to get a paying job out of the deal. And I won't do a complete concrete work-up for free, those run $1,000 and up. But I'd say just traveling 3 hours to look at a problem and then back and returning a couple times does cost me a fair amount of money, especially if I have to take an employee along. Most of the clients I have met are really good though. Remember I don't do residential work, and that's where a lot of the tire kickers are.... Wink

JD Grafton
Concrete Answers for Flooring Problems
JGrafton@ccsolves.com

Thomas55brien Show this Post
04-05-2011, 05:21 AM #9
Thomas55brien Unregistered
 
Can anyone explain what is the meaning of RH Testing?
Not familiar with the term.

04-05-2011, 05:33 AM #10
CC Solutions Concrete Moisture Evangelist *******
Status: Offline Posts:1,067 Threads:69 Joined:Dec 2009
(04-05-2011, 05:21 AM)Thomas55brien Wrote:  Can anyone explain what is the meaning of RH Testing?
Not familiar with the term.

In this context RH testing refers to In-Situ Relative Humidity testing, a process that follows ASTM F2170 which entails inserting a probe into the concrete to measure the amount of moisture in the concrete.

JD Grafton
Concrete Answers for Flooring Problems
JGrafton@ccsolves.com








Possibly Related Threads...
Thread / Author Replies / Views Last Post
4 Replies 15,434 Views
Last Post by Ashok Kakade
05-20-2014, 12:00 PM
2 Replies 12,759 Views
Last Post by eaadams
09-27-2013, 10:26 AM
33 Replies 100,477 Views
Last Post by eaadams
11-21-2012, 10:19 AM
51 Replies 167,387 Views
Last Post by ILLENTINC
11-19-2012, 11:59 AM
4 Replies 18,831 Views
Last Post by CC Solutions
09-18-2012, 06:11 PM
22 Replies 66,184 Views
Last Post by Ernesto
07-30-2012, 07:01 PM
36 Replies 122,139 Views
Last Post by CC Solutions
04-19-2011, 04:59 PM
2 Replies 14,128 Views
Last Post by eaadams
09-30-2010, 08:27 AM
11 Replies 43,823 Views
Last Post by CC Solutions
09-20-2010, 03:01 PM
15 Replies 55,235 Views
Last Post by Ernesto
01-12-2010, 10:56 AM

Users browsing this thread:
1 Guest(s)