Concrete Moisture Meters vs. Relative Humidity Testing
When it comes to flooring installation on a concrete slab, a critical aspect often overlooked is moisture management. Knowing the precise moisture levels within your concrete is more than just good practice—it’s key to preventing future flooring failures and ensuring the longevity of your installation.
However, the question remains: How should you measure this moisture?
This comprehensive guide will dissect the functionality of two popular moisture-measuring methods: Concrete Moisture Meters and Relative Humidity Testing. We’ll also address some burning questions, such as:
- Do Moisture Meters Work on Concrete
- Using a Moisture Meter on Concrete
- Measuring Relative Humidity in Concrete
- Relative Humidity and Concrete Moisture Content
- The Best Way to Test Concrete Moisture
- Concrete Moisture Meter Verdict
This article aims to debunk myths, provide insights, and guide building professionals and homeowners to make informed decisions about moisture control in concrete. After all, making the right choice could mean the difference between a durable floor that lasts for years and a disaster waiting to happen.
Concrete moisture meters should never be used to make the final determination as to whether or not a concrete slab is dry enough for a flooring installation.
Whether you’re a building professional or a homeowner, using the right tools and methods to measure and control moisture in concrete is essential for ensuring the longevity and durability of your floors.
Do Moisture Meters Work on Concrete
Yes, concrete moisture meters work. But no concrete moisture meter of any type can give consistently accurate concrete moisture meter readings across the different mixes and densities of concrete. Other components (metal reinforcing bar, aggregate size, amount, etc.) can also cause false indications of moisture.
Using a Moisture Meter on Concrete
The C555 pinless moisture meter effectively measures moisture in concrete on the top ½ inch of smooth slabs.
Pin-type meters are not practical for measuring moisture in concrete because variable chemical and physical characteristics can cause false moisture readings. This is due to changes in electrical resistance that have nothing to do with moisture.
However, remember that surface moisture meters provide readings only from the uppermost layer of the concrete, which may not be sufficient to assess moisture conditions throughout the slab. For a more accurate understanding of moisture conditions within a concrete slab, it’s best to use RH testing methods.
Measuring Relative Humidity in Concrete
Professionals typically use in-situ probes or sensors to measure the relative humidity (RH) within a concrete slab. The process involves drilling a hole into the concrete slab, often about 40% of the slab’s thickness for an on-grade or above-grade slab.
Once drilled, an in-situ probe is inserted into the hole. This probe measures the humidity deep within the slab and provides a percentage-based RH reading. The percentage indicates how much moisture is in the air inside the concrete compared to the maximum amount of moisture the air could hold at the same temperature.
Relative Humidity and Concrete Moisture Content
While “relative humidity” and “moisture content” may sound similar, it’s important to distinguish between the two. RH refers to the moisture level in the air, specifically inside the concrete slab, and is expressed as a percentage.
On the other hand, moisture content generally refers to the total amount of water in the concrete itself, often calculated by weight.
The Best Way to Test Concrete Moisture
The in-situ relative humidity (RH) testing method is the most reliable way to test concrete moisture. It provides an accurate measurement of the final moisture condition of the slab if it were sealed with a flooring product at that time.
The ASTM F2170 standard, which specifies the RH testing method, is recognized by flooring and adhesive manufacturers as the most accurate way to test concrete moisture. This method inserts RH sensors into the concrete slab, providing a precise understanding of how much moisture is present.
Additionally, concrete moisture meters were sufficiently accurate (again, they are not). They only measure ‘moisture’ (not relative humidity) in a small area near the concrete slab’s surface. This type of surface ‘moisture’ testing tells us nothing about the conditions down in the slab.
Once a floor covering is placed on a concrete slab, the relative humidity in the concrete slab will equilibrate throughout the thickness of the slab.
Meaning a slab that may have been “dry” (low RH) at the surface (without a floor covering) will see a higher RH at the surface when the floor covering has been installed. This is where the problems occur. The calcium chloride test method (moisture vapor emission) and the UK-based ‘hood’ method (RH) have the same problem, as they are also surface tests.
The calcium chloride test method (moisture vapor emission) and the UK-based ‘hood’ method (RH) have the same problem, as they are also surface tests.
Remember that an uncovered concrete slab will have an RH gradient throughout its thickness until a floor covering is put on top. Under normal conditions, the RH at roughly 50% slab depth will be significantly higher than the surface. Unless the slab has been down for a long time and a vapor retarder is directly underneath the slab.
In reality, the surface of the concrete will more closely reflect the RH in the room or building. This does not indicate the potential for a concrete flooring failure due to the high RH deep in the slab. That RH will migrate to the surface when the concrete can no longer emit water vapor due to the non-permeable floor covering.
Free Download – 4 Reasons Why Your Concrete Is Taking Forever to Dry
Again, most major floor covering and flooring adhesive manufacturers in North America and Europe already have concrete RH specifications in their installation guidelines.
Concrete Moisture Meter Verdict
At best, concrete moisture meters may have some practicality as relative (qualitative, not quantitative) measurement devices for possibly indicating the best placement for accurate, quantitative RH sensors within the concrete. Unlike other non-quantitative test methods, moisture meters for concrete are not final determination tools.
Learn more about RH probes.
So how can you ensure harmony between RH and MC?
Allow time for gradual acclimation when wood is moved to a new job site or location, particularly with exotic woods or woods that originated in markedly different climates. Or, if you have your own shop kiln for drying wood, set it for moderate changes over an extended schedule.
Monitor the changes with an accurate wood moisture meter.
Wood moisture meters from Wagner Meters provide easy, accurate, damage-free moisture measurement that lets you quickly determine MC of wood.
They also have the unique advantage of not being skewed by surface moisture. When RH is high and temperatures are cooler, a thin layer of condensation can form on the wood’s surface. Wagner’s IntelliSenseTM Technology reads past that moisture layer to provide a true picture of the wood’s internal MC.
Wood moisture meters can also be effective tools for determining unseen moisture-related problems in wood floors or other site materials where a change in MC could mean a water intrusion is in contact with the wood itself.
When RH and MC are in balance, your wood will perform at its best and retain its strength and beauty for years to come. Wood moisture meters from Wagner Meters provide a simple and effective way to determine when wood has reached a point of equilibrium with the RH of its environment.
As Sales Manager for Wagner Meters, Ron has more than 35 years of experience with instrumentation and measurement systems in different industries. In previous positions, he has served as Regional Sales Manager, Product and Projects Manager, and Sales Manager for manufacturers involved in measurement instrumentation.
Last updated on August 4th, 2023
I’m looking for an acceptable way to read moisture in concrete block (CMUs) walls. Our FL condo was hit by the eye of Hurricane Ian. I’m on the 6th floor with a total of seven floors. The roof had more than 100 punctures and the roof is being replaced. We have a dehumidifier and 4 air scrubbers in our 3BR and 3-bath condo (1850 square feet). Two feet of the gypsum board is removed under two windows. The humidity levels in the air are excellent (20-40%), especially for SW Florida.
My question is…what is the best way to measure moisture in the exposed CMU block wall? What should the percent moisture read with the masonry nails into the CMU?
The company has used these 3 methods:
1. The infrared thermography reads no moisture in the block or drywall.
2. The concrete moisture reader reads all but no moisture in the block (about 1 %).
3. Drilling stainless screws into the CMU. These are driven in at different depths of the block, creating an inconsistent depth of readings. The moisture reader reads from 8% to 11%. What are the pros and cons of using masonry nails?
Thank you,
Bonnie
I’m a 1st floor condo owner in Florida. My exterior walls and ceilings are concrete. I’m noticing stains on ceiling where exterior wall meets my ceiling. I just had house painted. Used Regal primer and Benjamin Moore Waterborne ultra flat ceiling paint. The areas of concern are below the upstairs terraces. I had inspection today and was told no way to test for moisture in concrete ceiling where it meets exterior stucco wall. Doesn’t sound right. Any suggestions?
Helene:
If I am understanding you correctly, it would be difficult to test the moisture in the corner where the two plains intersect. That being said, taking readings with a non-invasive concrete moisture meter around the areas that seem to be affected and comparing those to areas that seem to be performing well might shed light on whether elevated moisture may be causing the staining issues. Good luck.
We are replacing my flooring on my 1st floor. We removed 3 types of flooring, laminate floating floor, ceramic tile and engineered hardwood. The new floor would be all porcelain tile over the concrete slab. The installer used an electrical impedance meter to measure the moisture in the slab. Reading ranged from 3’s to 6’s. He wants to put down a vapor barrier on the concrete slab before installing the porcelain tile. The distributor said we could use a product called Red Guard but he said that is not a vapor barrier. I contacted the company that makes Red Guard and they said it can be used as a vapor barrier when the moisture is not more than 12 pounds per thousand square ft. What are your thoughts?
Marie:
Thanks for the question. In order for you to meet the Red Guard specification, you will need to perform a calcium chloride test on the concrete. This is one of only two widely recognized moisture testing methods for concrete, the other being relative humidity testing. Good luck.
We moved into a new build home on Feb 28, 2020 and have noticed the vinyl plank flooring starting to chip and break. The flooring company came out and did a pin meter moisture test is a couple of areas beneath the vinyl and carpeting in different parts of the home. Under the vinyl the meter was maxed and under the carpet it was mid 80% reading, I purchased a meter at Lowes and checked it and got a 100% vinyl reading and 82-87% reading under the carpet. Since we closed and moved in Feb the slab is less than a year old, we do you recommend? We are still under warranty and do you think we may have serious foundation issues.
Thank you, Clay
Clay:
Thank you for the questions. First for the meter readings you describe. A pin meter isn’t the industry standard for testing moisture in concrete for the purposes of installing flooring, so I can’t really judge the numbers you have provided. I can state though that I have never heard of moisture in concrete causing chipping or breaking of vinyl plank. Secondly, based on any information you have provided here, I see no reason to think there is an issue with your foundation. Good luck.
What is a concrete moisture content on meters?
On a range from 0-6 what is an acceptable reading to install? Im confused on that. Help please!!!
Carlos,
The meters you are referencing aren’t really intended to make absolute decisions on installations, they are intended to identify hot spots on a given floor where you should do accepted tests like calcium chloride and relative humidity tests. That being said, in the wood flooring installation world, there are some adhesive companies that do recognize this type of testing, but you would have to consult them for acceptable numbers. Good luck.
is 75% a typical RH level for a coatable concrete floor?
Mike,
Thanks for the question. Many of the coatings manufacturer’s I see have a 75% maximum listed. Some of the more cutting-edge companies may have a higher number because they have done testing to confirm they can go higher. In any event, ALWAYS check with the individual manufacturer for their specific information.
Hi Jason,
I am work at applicator of flooring paint. In the technical data sheet of two suppliers differ in concrete moisture content :
+ Substrate moisture content is between 4% to 6%.
+ The other is Substrate moisture content within 75% RH
Can you show me the relationship of these two quantities? And can I convert them together?
Thank you!
Nong:
Thanks for the question. The 4-6% is usually measured with a surface moisture meter and the 75% RH is usually measured with a device such as http://www.rapidrh.com. Being two different testing methodologies, there are no conversions.
I loved this blog, and this blog provides all the information that is required to know about concrete moisture. All my queries about this equipment got solved after reading this. Keep it up.
Hi Jason
The moisture readings obtained from the meters would effectively be meaningless.
In water damage situations depending on the amount and head of water the depth to which the moisure has been absorbed will vary greatly.
When called upon to test the moisture readings it would be advisable to add a disclaimer and advise the flooring supplier should satisfy himself if the concrete moisure content is within acceptable range. The relative humidity test determined by driling holes would be most appropriate. However the down side is that its time consuming and could be expensive, although the expense should be minor consideration compared to the cost for replacement of a failed floor covering.
Pammy
AH right? ahwile back i did a laminate install over concrete where carpet and pad was removed……pin type moisture readings were about 3% average which is acceptable……two months later the floor failed due to moisture. we figured the reason was is because the carpet and pad allowed to concrete to breath to a certain exten,t after installing the laminate it covered and sealed to floor so to speak then the moisture deep in the concrete had no where to go and caused the floor to fail. so much for pin type moisture meter (Tramex CME 4) was used.
Patrick
Patrick:
Thanks for the comment and very good observations. This is one reason that surface meters are intended for scanning of a concrete floor surface and not intended, per ASTM F2659, to be used to make an installation decision.
Thanks,
Jason
Does this same info apply if the subfloor is 1 1/4″ gypcrete that is being asked to seal when moisture meter reading says 26%
can you RH test a 1 14/” gypcrete level?
Stacy:
Thanks for the question. The best way to answer this question is by contacting the gypcrete manufacturer and the flooring and adhesive manufacturer. They should be able to give you specific guidance on this that would cover their specific warranties.
Thanks,
Jason
Ron,
I would like to assess the effect of surface moisture on spray foam adhesion. Wood is fairly straight forward, but I am not sure what the right method and device is for the surface of concrete. I recently observed an application where the horizontal ceiling slab delaminated, while the vertical walls were well bonded. Thank you for any advice you can provide on making sure the substrate is ready before the installer begins his work.
Henri, I think it would be best if we could discuss this over the phone. You can call 1-800-634-9961 and ask for me specifically. Our office hours are 7:30am to 4:00pm PT, Monday through Friday. Thanks.