50% fail rate

#6
Revisiting this thread and I was just thinking that if the probes were cold and put into a warm slab there could be condensation forming on the sensor which will mess with readings.... Typically this is something we need to worry about in the north, not so much in southern climes.
JD Grafton
Concrete Answers for Flooring Problems
[email protected]
Reply


Messages In This Thread
50% fail rate - eaadams - 05-27-2011, 10:55 AM
RE: 50% fail rate - EWagner - 05-27-2011, 03:55 PM
RE: 50% fail rate - eaadams - 05-27-2011, 04:57 PM
RE: 50% fail rate - CC Solutions - 05-30-2011, 11:18 AM
RE: 50% fail rate - eaadams - 05-30-2011, 01:24 PM
RE: 50% fail rate - CC Solutions - 09-12-2011, 05:43 PM
RE: 50% fail rate - eaadams - 09-13-2011, 03:07 PM
RE: 50% fail rate - CC Solutions - 09-13-2011, 05:44 PM
RE: 50% fail rate - eaadams - 09-13-2011, 05:50 PM
RE: 50% fail rate - CC Solutions - 09-13-2011, 05:58 PM
RE: 50% fail rate - eaadams - 09-13-2011, 06:01 PM
RE: 50% fail rate - CC Solutions - 09-13-2011, 06:04 PM

Digg   Delicious   Reddit   Facebook   Twitter   StumbleUpon  


Users browsing this thread:
1 Guest(s)