All tests done with Wagner 4.0.

Date / test site / RH / Temp

7-11 / #1 / 94 / 73
7-17 / #1 / 94 / not recorded
[heat turned on, air moved, floor received a light shotblast to a CSP of no more than 2]
7-30 / #1 / 94 / 79
8-07 - no test

7-11 / #2 / 96 / 73
7-17 / #2 / 91 / not recorded
[heat turned on, air moved, floor received a light shotblast to a CSP of no more than 2]
7-30 / #2 / [no reading / debris]
[hole vacuumed out of debris @ time of test]
8-07 - no test

7-11 / #3 / 91 / 74
7-17 / #3 / 99 / not recorded
[heat turned on, air moved, floor received a light shotblast to a CSP of no more than 2]
7-30 / #3 / 99 / 79
8-07 / #3 / 94 / 76

7-11 / #4 / 92 / 72
7-17 / #4 / 92 / not recorded
[heat turned on, air moved, floor received a light shotblast to a CSP of no more than 2]
7-30 / #4 / 91 / 79
8-07 / #4 / 91 / 75

7-11 / #5 / 99 / 72
7-17 / #5 / 99 / not recorded
[heat turned on, air moved, floor received a light shotblast to a CSP of no more than 2]
7-30 / #5 / 94 / 79
8-07 - no test


Obviously the slab temp went up when we cranked the HVAC. I think removing the old adhesive with the light shotblast helped a lot to let moisture out just over one month.
Reply

#2
You had three 'no-tests' on 8/7. It would help to see what those probes read.

Were the probes acclimated for 72 hours on the first test date of 7/11? If not we should discount those readings.

When the slab temp rises we expect to see a decrease in relative humidity. Additional readings would help indicate a trend. Another helpful bit of information would be ambient conditions and whether the HVAC is constantly on or just being run sporadically. Is the building envelope completed and sealed?
JD Grafton
Concrete Answers for Flooring Problems
[email protected]
Reply


Possibly Related Threads...
Thread Author Replies Views Last Post
  low and high moisture readings affected by air RH jpsflooring 9 3,871 04-16-2014, 03:49 PM
Last Post: Ernesto
  RH test results varying Erica 7 14,963 05-09-2012, 04:35 PM
Last Post: Rubensgt40
Question false high test results eaadams 11 25,327 10-28-2011, 02:12 PM
Last Post: CC Solutions

Digg   Delicious   Reddit   Facebook   Twitter   StumbleUpon  


Users browsing this thread:
1 Guest(s)