(04-18-2011, 12:26 PM)T_Schneider Wrote:  COD, I realize I am showing up very late to this party, but I did want to point out that ASTM F2170 requires the space to be acclimated (HVAC on) prior to testing for relative humidity. This may have been skewing your data.

Regards,

T. Schneider
ARDEX Engineered Cements

Technically nowhere in the ASTM does it say the space must have the HVAC on.

We wouldn't want testers thinking they cannot conduct accurate RH testing just because the HVAC is not on. In 99% of all the hospitals I work in, the HVAC is not commissioned until a few days before the building is turned over.

JD Grafton
Concrete Answers for Flooring Problems
JGrafton@ccsolves.com








Messages In This Thread
RH Numbers Rising - COD - 04-05-2011, 09:40 AM
RE: RH Numbers Rising - eaadams - 04-05-2011, 10:49 AM
RE: RH Numbers Rising - Ernesto - 04-05-2011, 11:49 AM
RE: RH Numbers Rising - eaadams - 04-05-2011, 12:19 PM
RE: RH Numbers Rising - Ernesto - 04-05-2011, 12:27 PM
RE: RH Numbers Rising - COD - 04-05-2011, 01:16 PM
RE: RH Numbers Rising - CC Solutions - 04-05-2011, 05:26 PM
RE: RH Numbers Rising - Ernesto - 04-05-2011, 08:42 PM
RE: RH Numbers Rising - CC Solutions - 04-06-2011, 06:04 AM
RE: RH Numbers Rising - Ernesto - 04-06-2011, 07:40 AM
RE: RH Numbers Rising - CC Solutions - 04-06-2011, 07:47 AM
RE: RH Numbers Rising - Ernesto - 04-06-2011, 08:23 AM
RE: RH Numbers Rising - CC Solutions - 04-06-2011, 08:28 AM
RE: RH Numbers Rising - Ernesto - 04-06-2011, 04:54 PM
RE: RH Numbers Rising - CC Solutions - 04-07-2011, 06:12 AM
RE: RH Numbers Rising - rthompson - 04-07-2011, 01:08 PM
RE: RH Numbers Rising - Ernesto - 04-08-2011, 08:01 AM
RE: RH Numbers Rising - CC Solutions - 04-08-2011, 08:06 AM
RE: RH Numbers Rising - rthompson - 04-08-2011, 10:33 AM
RE: RH Numbers Rising - eaadams - 04-08-2011, 04:19 PM
RE: RH Numbers Rising - Ernesto - 04-08-2011, 04:54 PM
RE: RH Numbers Rising - eaadams - 04-08-2011, 05:00 PM
RE: RH Numbers Rising - CC Solutions - 04-09-2011, 08:59 AM
RE: RH Numbers Rising - rthompson - 04-09-2011, 11:57 AM
RE: RH Numbers Rising - CC Solutions - 04-09-2011, 01:14 PM
RE: RH Numbers Rising - eaadams - 04-09-2011, 01:38 PM
RE: RH Numbers Rising - CC Solutions - 04-09-2011, 01:46 PM
RE: RH Numbers Rising - rthompson - 04-09-2011, 02:06 PM
RE: RH Numbers Rising - CC Solutions - 04-09-2011, 02:39 PM
RE: RH Numbers Rising - Ernesto - 04-11-2011, 09:49 AM
RE: RH Numbers Rising - CC Solutions - 04-11-2011, 09:54 AM
RE: RH Numbers Rising - Ernesto - 04-11-2011, 08:50 PM
RE: RH Numbers Rising - T_Schneider - 04-18-2011, 12:26 PM
RE: RH Numbers Rising - CC Solutions - 04-18-2011, 01:10 PM
RE: RH Numbers Rising - T_Schneider - 04-18-2011, 01:20 PM
RE: RH Numbers Rising - CC Solutions - 04-18-2011, 01:28 PM
RE: RH Numbers Rising - Ernesto - 04-18-2011, 03:08 PM
RE: RH Numbers Rising - eaadams - 04-18-2011, 04:46 PM
RE: RH Numbers Rising - Ernesto - 04-18-2011, 04:55 PM
RE: RH Numbers Rising - CC Solutions - 04-18-2011, 05:15 PM
RE: RH Numbers Rising - Ernesto - 04-20-2011, 07:58 AM
RE: RH Numbers Rising - CC Solutions - 04-20-2011, 08:02 AM
RE: RH Numbers Rising - rthompson - 04-20-2011, 05:15 PM
RE: RH Numbers Rising - CC Solutions - 04-20-2011, 09:00 PM
RE: RH Numbers Rising - Ernesto - 04-23-2011, 07:01 PM
RE: RH Numbers Rising - rthompson - 04-23-2011, 07:59 PM
RE: RH Numbers Rising - CC Solutions - 04-23-2011, 08:59 PM
RE: RH Numbers Rising - rthompson - 04-23-2011, 10:01 PM
RE: RH Numbers Rising - Ernesto - 04-24-2011, 08:24 AM
RE: RH Numbers Rising - eaadams - 09-08-2011, 06:08 PM
RE: RH Numbers Rising - CC Solutions - 09-09-2011, 08:11 AM
RE: RH Numbers Rising - rthompson - 09-09-2011, 09:36 AM
RE: RH Numbers Rising - Ernesto - 09-09-2011, 04:48 PM
RE: RH Numbers Rising - CC Solutions - 09-10-2011, 07:47 AM
RE: RH Numbers Rising - Ernesto - 09-10-2011, 11:14 AM
RE: RH Numbers Rising - CC Solutions - 09-10-2011, 06:30 PM
RE: RH Numbers Rising - Ernesto - 09-11-2011, 08:22 AM
RE: RH Numbers Rising - rthompson - 09-11-2011, 08:25 AM
RE: RH Numbers Rising - Ernesto - 09-11-2011, 08:40 AM
RE: RH Numbers Rising - CC Solutions - 09-11-2011, 03:54 PM
RE: RH Numbers Rising - Ernesto - 09-11-2011, 06:50 PM
RE: RH Numbers Rising - rthompson - 09-12-2011, 08:56 AM
RE: RH Numbers Rising - CC Solutions - 09-12-2011, 09:07 AM
RE: RH Numbers Rising - Ernesto - 09-12-2011, 05:14 PM
RE: RH Numbers Rising - CC Solutions - 09-12-2011, 05:33 PM
RE: RH Numbers Rising - Ernesto - 09-12-2011, 07:27 PM
RE: RH Numbers Rising - CC Solutions - 09-13-2011, 05:52 AM
RE: RH Numbers Rising - Ernesto - 09-13-2011, 07:49 AM
RE: RH Numbers Rising - rthompson - 09-13-2011, 08:37 AM
RE: RH Numbers Rising - CC Solutions - 09-13-2011, 08:43 AM
RE: RH Numbers Rising - Ernesto - 09-13-2011, 10:08 AM
RE: RH Numbers Rising - CC Solutions - 09-13-2011, 11:28 AM
RE: RH Numbers Rising - Ernesto - 09-13-2011, 01:37 PM
RE: RH Numbers Rising - CC Solutions - 09-13-2011, 01:55 PM
RE: RH Numbers Rising - eaadams - 09-13-2011, 02:14 PM
RE: RH Numbers Rising - Ernesto - 09-13-2011, 02:17 PM
RE: RH Numbers Rising - eaadams - 09-13-2011, 02:18 PM
RE: RH Numbers Rising - CC Solutions - 09-13-2011, 02:33 PM
RE: RH Numbers Rising - Ernesto - 09-13-2011, 05:26 PM
RE: RH Numbers Rising - eaadams - 09-13-2011, 05:46 PM
RE: RH Numbers Rising - CC Solutions - 09-13-2011, 05:52 PM
RE: RH Numbers Rising - eaadams - 09-13-2011, 05:56 PM
RE: RH Numbers Rising - CC Solutions - 09-13-2011, 06:03 PM
RE: RH Numbers Rising - eaadams - 09-13-2011, 06:06 PM
RE: RH Numbers Rising - Ernesto - 09-13-2011, 07:23 PM
RE: RH Numbers Rising - Ernesto - 09-14-2011, 06:29 AM
RE: RH Numbers Rising - CC Solutions - 09-14-2011, 06:54 AM
RE: RH Numbers Rising - Ernesto - 09-14-2011, 07:39 PM
RE: RH Numbers Rising - CC Solutions - 09-15-2011, 04:59 AM
RE: RH Numbers Rising - Ernesto - 09-20-2011, 08:07 PM
RE: RH Numbers Rising - CC Solutions - 09-20-2011, 08:30 PM
RE: RH Numbers Rising - Ernesto - 09-21-2011, 08:19 PM
RE: RH Numbers Rising - CC Solutions - 09-21-2011, 09:18 PM
RE: RH Numbers Rising - eaadams - 09-22-2011, 08:39 AM
RE: RH Numbers Rising - CC Solutions - 09-22-2011, 09:28 AM
RE: RH Numbers Rising - Ernesto - 09-22-2011, 07:14 PM
RE: RH Numbers Rising - eaadams - 09-22-2011, 07:50 PM
RE: RH Numbers Rising - Ernesto - 09-22-2011, 08:00 PM
RE: RH Numbers Rising - eaadams - 09-22-2011, 08:48 PM
RE: RH Numbers Rising - CC Solutions - 09-23-2011, 05:54 AM
RE: RH Numbers Rising - Ernesto - 09-23-2011, 06:58 AM
RE: RH Numbers Rising - CC Solutions - 09-23-2011, 10:37 AM

Users browsing this thread:
1 Guest(s)